Details

Purifying?agent?for?molten?zinc?in?HDG
Name:
Purifying?agent?for?molten?zinc?in?HDG
  • Model:
  • Uses:
  •  
Details

In the light of the high iron and impurity contents in molten zinc, poor fluidness and particles and fold on workpiece often occurred in hot galvanizing plants, our company has organized the famous specialists and scientific and technological personnel in many disciplines at home developed XY-XG-3 type purifying agent for molten zinc, a high and new technical product. It has effectively solved the difficult problem and filled in the gap in this field at home. Through testing and using, the agent reached the anticipated results and is well received by customers. At present the product is applying for a patent. 
Notice
Do well pretreatment work, do not carry the harmful impurity into zinc pot, galvanizing agent needs the acid and iron eliminating, and it would be best if rinsing water for pretreatment could be fluid.
Because of the high volatility of the agent, No.2 operation should be quickly performed.
In order to avoid the splashing of molten zinc causing danger, operators should be well dressed in labor protection articles. Operation with caution and safety first.
Purifying Treatment Method of Molten Zinc:
Keep furnace temperature at 450℃-470℃.
Place dry thermal insulation bricks (with strong water absorption) into box with holes, quickly pour the purifying agent to them, insert the box into molten zinc and move it back and forth until boiling ends, and take out the box with holes.
Eliminate suspended substances on the surface of molten zinc; scatter ammonium chloride (1-1.5 kg/ m2) to further eliminate impurity on the surface.
Repeat the abovementioned steps three or four times.
Add the alloy, which is 0.5% of molten zinc, in uniform distribution way. After all the melting, repeat the abovementioned step once. (If there are excessive aluminum or other alloys in original molten zinc, the step-by-step method can be used)
The temperature is controlled at 430℃-440℃ and the standing time is 6-12 h (time is as long as possible).
When small workpiece is tested (the temperature is at 430℃ and dipping time is not changed), the surface and coating thickness is measured. If the coating is thick, the alloy, which is 0.1 % of molten zinc, can be added. 
The zinc and the alloy can be added at one time until the alloy content in molten zinc reaches 1.5%.
After alloying is completed, the working temperature of molten zinc should be controlled at 440℃±5℃ and the lifting speed of traveling crane at 1.5 m / min.
 

 

返回頂部 電話
主站蜘蛛池模板: 国产日韩一区二区三区| 欧美国产日韩在线| 成人性做爰aaa片免费看曹查理| 91射射射| 久久久久亚洲| 中文字幕丰满乱子无码视频| 美女久久久久| 狼色精品人妻在线视频免费| 最新亚洲视频| 一级片观看| 人人妻人人澡人人爽欧美一区 | 丁香成人影院| 丰满少妇被猛烈进av毛片| 男女啪动最猛动态图| 午夜dj在线观看神马视频| 国产无遮挡又黄又爽高潮| 91免费公开视频| 欧美大黑bbb| 无码人妻精品一区二区三区东京热 | 精品人妻va出轨中文字幕| www日日日| 久久婷婷av| 久久精品伊人波多野结衣| 嫩嫩草网站| 日本aⅴ在线观看| a毛看片免费观看视频| 无码无套少妇毛多18pxxxx| 中文字幕 国产| 亚洲国产综合人成综合网站00| 国产精品毛片av在线看| 国产xxx在线观看| 午夜草逼| 色偷偷噜噜噜亚洲男人| 亚洲精品乱码久久久久久金桔影视| 日韩有码在线观看| 二级黄| 精品无码av不卡一区二区三区| 日韩美在线| 一级毛片视频在线观看| 欧美日韩高清不卡一区二区三区| 久久久成人毛片无码|